Nominal chemical composition % (to EN 573-1):
|
|
Si
|
Fe
|
Cu
|
Zn
|
Remarques
|
Others
|
Al
|
| Each |
Total |
| 0,4 |
0,7
|
5,0-6,0 |
0,3
|
0,2-0,6 Bi; 0,2-0,6 Pb
|
0,05
|
0,15
|
Remainder |
|
|
Typical mechanical properties:
|
|
Bars extruded (to EN 755-2):
|
|
Temper
|
Dimensions (mm)
|
Rm (MPa)
|
Rp0,2 (MPa)
|
A%
|
A50 %
|
|
Diam
|
Across flats
|
Mini
|
Mini
|
Mini
|
Mini
|
|
T4
|
<200
|
<60
|
275
|
125
|
14
|
12
|
|
T6
|
<75
75 to 200
|
<60
-
|
310
295
|
230
195
|
8
6
|
6
|
|
|
Tubes extruded (to EN-755-2) :
|
|
Temper
|
Dimensions mm
Wall thickness
|
Rm (MPa)
|
Rp0,2 (MPa)
|
A % mini
|
A50 % mini
|
|
mini
|
max
|
mini
|
max
|
|
T6
|
£ 25
|
310
|
-
|
230
|
-
|
6
|
4
|
|
|
Bars drawn (to EN-754-2) :
|
|
Temper
|
Dimensions mm
|
Rm (MPa)
|
Rp0,2 (MPa)
|
A % mini
|
A50 % mini
|
|
Diameter (D)
|
Across flats or thickness (S)
|
mini
|
max
|
mini
|
max
|
|
T3
|
£ 40
40<D£ 50
50<D£ 80
|
£ 40
40<S£ 50
50<S£ 80
|
320
300
280
|
-
-
-
|
270
250
210
|
-
-
-
|
10
10
10
|
8
-
-
|
|
T8
|
£ 80
|
£ 80
|
370
|
-
|
270
|
-
|
8
|
6
|
|
|
Tubes drawn (to EN-754-2) :
|
|
Temper
|
Dimensions mm
Wall thickness
|
Rm (MPa)
|
Rp0,2 (MPa)
|
A % mini
|
A50 % mini
|
|
mini
|
max
|
mini
|
max
|
|
T3
|
£ 5
5<e£ 20
|
310
290
|
-
-
|
260
240
|
-
-
|
10
8
|
8
6
|
|
T8
|
£ 20
|
370
|
-
|
275
|
-
|
8
|
6
|
|
|
Wire (to EN 1301-2):
|
|
Temper
|
Diameter up to and including
|
Rm (MPa)
|
Rp0,2 (MPa)
typical
|
A100 m % typique
|
|
mini
|
max
|
|
T3
|
18
|
310
|
-
|
295
|
6
|
|
T8
|
18
|
370
|
-
|
310
|
4
|
|
|
Properties (for guidance only):
|
|
Corrosion:
|
| General corrosion rating |
Not recommended
|
| Corrosion in industrial atmosphere |
Not recommended
|
| Corrosion in marine atmosphere |
Not recommended
|
| Corrosion in rural atmosphere |
Acceptable
|
| Stress corrosion |
Not recommended
|
| Exfoliation rating |
Acceptable
|
| Intergranular corrosion |
Acceptable
|
| Pitting rating |
Not recommended
|
|
|
Anodising:
|
| Bright anodising |
Not recommended
|
| Colour anodising |
Not recommended
|
| Hard anodising |
Good
|
| Protective anodising |
Acceptable
|
|
|
Forming, machining:
|
| |
Ecrouis
|
| Cold forming |
Not recommended to strongly discouraged
|
| Deep drawing |
Not recommended
|
| Stretch forming |
Not recommended
|
| Spinning ability |
Strongly discouraged
|
| Extrudability |
Good
|
| Machinability |
Excellent
|
|
|
Welding:
|
| Electron beam welding |
-
|
| Gas welding |
Strongly discouraged
|
| Arc welding |
Strongly discouraged
|
| Spot welding |
Not recommended
|
| Brazing |
Not recommended
|
| Soft soldering |
Acceptable
|
|
|
Physical and elastic properties:
|
|
Temper
|
Elastic
|
Physiques
|
| |
E
|
G
|
n
|
Tsol
|
Tliq
|
Cp
|
a
|
r
|
rel
|
l
|
EC
|
|
MPa
|
MPa
|
-
|
°C
|
°C
|
J kg-1 K-1
|
µm m-1 K-1
|
kg m-3
|
nW m
|
W m-1 K-1
|
%IACS
|
|
T3 / T4
|
72500
|
27300
|
0.33
|
540
|
645
|
863
|
23
|
2840
|
44
|
152
|
39
|
|
T6 / T8
|
72500
|
27300
|
0.33
|
540
|
645
|
863
|
23
|
2840
|
38
|
172
|
45.5
|
|
| Key: |
|
E
|
Modulus of elasticity |
MPa |
|
G
|
Modulus of rigidity |
MPa |
|
n
|
Poisson's ratio |
|
|
Tsol
|
Solidus temperature |
°C |
|
Tliq
|
Melting temperature |
°C |
|
Cp
|
Specific heat |
J kg-1 K-1 |
|
a
|
Coefficient of thermal expansion |
µm m-1 K-1 |
|
r
|
Density |
kg m-3 |
|
rel
|
Resistivity |
nW m |
|
l
|
Thermal conductivity |
W m-1 K-1 |
|
EC
|
Electrical conductivity |
%IACS |
|
| International equivalents: |
|
International
|
France
|
Germany
|
Great Britain
|
Italy
|
Switzerland
|
Spain
|
|
AA
|
NFA
|
Former
|
DIN
|
WNR
|
BS
|
Former
|
UNI
|
Former
|
SNCH
|
UNE
|
|
2011
|
2011
|
AU5PbBi
|
AlCuBiPb
|
3.1655
|
-
|
FC1
|
9002/5
|
6362
|
AlCu6BiPb
|
L 3192
|
|
Sweden
|
Russia
|
USA
|
Japan
|
Canada
|
Australia
|
Czechoslovakia
|
Finland
|
Norway
|
Netherlands
|
|
SS
|
GOST
|
ASTM
|
JIS
|
Former
|
CSA
|
|
CSN
|
SFS
|
NS
|
|
|
4355
|
-
|
2011
|
A2011
|
-
|
28S / CB60
|
A2011
|
-
|
-
|
-
|
14/11
|
|